YLCE-2021 is a cycloaliphatic epoxy resin with two internal epoxy groups, an EEW of 125–135 g/eq and a viscosity of 200–300 mPa·s at 25 °C. Total chlorine is capped at 50 ppm and the cured ester network reaches a published Tg of up to 195 °C. Clear castings and UV-curable coatings are the main uses.

Figure 1. YLCE-2021 as delivered, 200–300 mPa·s at 25 °C. The bench reads through the beaker, which is the first test most receiving bays apply.
Alicyclic diepoxides sit apart from the bisphenol A family. YLCE-2021 carries two epoxy groups fused into cyclohexane rings and bridged by an ester link, so the reactive site is the ring, not a glycidyl ether tail.
That difference decides where the grade earns its price. An aromatic ring absorbs ultraviolet light and oxidises into coloured products; a saturated ring does not. Clear coatings start from alicyclic stock when colour drift matters.
This report fixes the published window, converts epoxide equivalent into hardener weight, and compares the grade with a glycidyl ester and a bisphenol A liquid. It also names the jobs the resin cannot do.
Table 1 holds the identity fields a purchase order needs. Table 2 holds the specification lines the supplier publishes, next to the fields left blank.
Table 1. Identity data for YLCE-2021 as published on the product page, accessed 2026-11-12.
Item |
YLCE-2021 |
Chemical name |
3,4-Epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate |
CAS number |
2386-87-0 |
Epoxide groups |
2, both internal (alicyclic) |
Appearance |
Colourless liquid |
Packaging |
Drums; IBC tanks |
Shelf life |
24 months from manufacture |
Storage |
5–30 °C, dry, out of sunlight |
Table 2. Published specification of the YLCE-2021 grade, with the test basis normally applied.
Item |
Published value |
Usual test basis |
Colour, Pt-Co |
Max. 50 |
ASTM D1544 |
Epoxy equivalent weight |
125–135 g/eq |
ASTM D1652 or ISO 3001 |
Viscosity at 25 °C |
200–300 mPa·s |
Rotational spindle; ASTM D445 for kinematic |
Total chlorine |
Max. 50 ppm |
Combustion and titration, method not stated |
Tg of cured casting |
up to 195 °C |
Supplier statement, method not stated |
Density |
Not published |
Request on TDS |
Water content |
Not published |
ASTM E203, Karl Fischer |
Flash point |
Not published |
ASTM D93 |
Three fields formulators ask for early are missing. None changes the stoichiometry, but density decides whether a 200 L batch fills the mould, and water above 0.05% slows a cationic cure.
Every value in Table 2 was read from the product page on 2026-11-12. The page does not name the titration behind the 125–135 g/eq window, so the window is a purchase specification, not one measurement.
Viscosity carries more uncertainty than a datasheet suggests. A 250 mPa·s liquid sits low on most spindles, where geometry and shear rate move the reading by several percent; duplicate runs agree only at a held 25 °C.
Calculated values come from the named structure and the published EEW. Field figures are labelled as such. A purchase decision should rest on a triplicate titration from the lot COA.
The named structure gives 252.31 g/mol for C14H20O4 and two epoxides, so the theoretical EEW is 126.2 g/eq. The published 125–135 g/eq window brackets that figure: the grade is close to a pure diepoxide.
Epoxy content follows at 0.74–0.80 eq per 100 g, against 0.53 eq per 100 g for a 187 g/eq bisphenol A liquid. That is 45% more reactive groups per kilogram, which is how a tight network forms at 250 mPa·s.
The internal epoxide also changes cure chemistry. Ring-opening runs through a cationic path, so strong acids and photogenerated acids start it fast under heat or ultraviolet light. Anhydrides need heat; aliphatic amines barely react.
Chlorine separates this grade from glycidyl ethers. Total chlorine is capped at 50 ppm, while the bisphenol A liquid YLE-128 permits 500 ppm hydrolyzable chlorine. Under humid bias, mobile chloride feeds ionic migration, so the cap matters in encapsulation.
Treat the 195 °C figure with care. Published Tg tracks the hardener and the schedule, and a casting held 2 h at 120 °C will miss a post-cured value. Confirm it by DMA on your own coupon.
Table 3 sets the grade against the two resins a buyer usually shortlists.
Table 3. Cycloaliphatic epoxy resin YLCE-2021 against YLCE-186 glycidyl ester and bisphenol A liquid grades.
Property |
YLCE-2021 |
YLCE-186 |
YLE-128 |
Epoxide type |
Alicyclic, ester bridge |
1 alicyclic + 2 glycidyl ester |
Glycidyl ether |
Functionality |
2 |
3 |
2 |
EEW, g/eq |
125–135 |
100–125 (186 / 186C) |
184–190 |
Viscosity, 25 °C |
200–300 mPa·s |
2,000–5,000 cps |
11,000–15,000 mPa·s |
Chlorine |
≤50 ppm total |
Not published |
≤500 ppm hydrolyzable |
Colour |
Pt-Co ≤50 |
APHA ≤50 |
Not published |
State |
Colourless liquid |
Colourless to light yellow |
Clear liquid |
YLCE-186 reacts faster with anhydrides, because two glycidyl esters join the alicyclic ring, but its viscosity runs eight to twenty times higher. YLE-128 costs less per kilogram and brings adhesion.
Read the columns as a process decision. Low viscosity buys filler loading; ester groups buy reactivity; aromatic rings buy toughness and price. None wins on all three.
Hardener weight follows from the epoxide equivalent: phr = 100 × AEW ÷ EEW, where AEW is the active hydrogen equivalent weight. A factor k of 0.80–0.90 is usual for anhydrides, and 0.85 suits MHHPA hardener in castings.
Table 4. Hardener demand across the published EEW window, calculated with MHHPA (AEW 168.19 g/eq) and DETA (AHEW 20.6 g/eq).
EEW, g/eq |
Epoxy content, eq/100 g |
MHHPA, k = 1.00 |
MHHPA, k = 0.85 |
DETA, phr |
125 |
0.80 |
134.6 phr |
114.4 phr |
16.5 |
130 |
0.77 |
129.4 phr |
110.0 phr |
15.8 |
135 |
0.74 |
124.6 phr |
105.9 phr |
15.3 |
Worked example at the mid-point: EEW 130 g/eq with MHHPA at 168.19 g/eq gives 129.4 phr at k = 1.00, or 110.0 phr at k = 0.85. A 500 g batch therefore takes 550 g of anhydride.
Amine hardeners look cheap on paper and behave badly here. DETA at 15.8 phr is stoichiometrically correct, yet the internal epoxide reacts slowly at room temperature and the film stays tacky for hours. A polyetheramine such as YLH-6005 curing agent at 73.1 phr cures, but only with heat.
Table 5. Viscosity and EEW of YLCE-2021 blended with bisphenol A liquid, estimated by the log-mixing rule at 25 °C.
YLE-128 share |
Blend EEW |
Viscosity estimate |
Practical effect |
0% |
130 g/eq |
250 mPa·s |
fastest wet-out |
10% |
134 g/eq |
370 mPa·s |
slight toughening |
20% |
138 g/eq |
550 mPa·s |
better adhesion to metal |
30% |
143 g/eq |
820 mPa·s |
cheaper, slower flow |
These are log-mixing estimates, not measurements. The trade-off is plain: 10% bisphenol A costs 50% more viscosity, and that is about all a casting shop absorbs.
Five habits keep a 250 mPa·s casting out of trouble.
• Hold the drum at 20–25 °C; at 15 °C viscosity doubles and de-airing drags.
• Meter anhydride by weight; density differences skew phr by 5%.
• Degas at 5–10 mbar for 10–15 min, in a shallow layer.
• Pre-heat the mould; a cold wall traps air at the surface.
• Dose 1–3 phr of cationic photoinitiator for UV work, and expect oxygen inhibition.

Figure 2. Pouring YLCE-2021 into an open mould. At 200–300 mPa·s the stream breaks cleanly and finds fine detail without vacuum.
Cationic cure is easily poisoned. Trace amine from an earlier batch, silicone release agent, or water above 0.05% will slow or stop it. The symptom is a tacky skin over a hard body: it reads as undercure and is contamination.
Table 6 ties each published use to the property that carries it.
Table 6. Published applications of YLCE-2021 and the property each one depends on.
Application |
Function of the resin |
Property that decides it |
Electrical casting |
Insulation and mechanical support |
Low viscosity fills fine windings |
LED packaging |
Optical path and protection |
Pt-Co ≤50, no aromatic ring |
Light-curing coating |
Fast ambient cure |
Cationic ring-opening under UV |
3D printing resin |
Photopolymer backbone |
Low viscosity at 25 °C |
Cable core composite |
Binder with low void content |
Wet-out at low pressure |
Insulation material |
Dielectric support, UV stability |
Saturated ring; UV and radiation resistance |

Figure 3. A cured YLCE-2021 casting around a threaded insert. Clarity of this order needs a filtered mix and a mould at cure temperature.
Two of those uses pull in opposite directions. Optical potting wants the lowest colour, electrical casting the lowest chlorine, and both point at one grade, so a single drum serves both lines. The YLSE-721 amine epoxy covers 200–260 °C structural work.
YLCE-2021 is the wrong choice in four situations, and each shows up in the first trial.
• Room-temperature amine cure: the internal epoxide reacts slowly, so a DETA system stays soft overnight.
• Hot caustic or strong acid service: the ester bridge hydrolyses before the part visibly discolours.
• Thick sections in one shot: low viscosity plus high exotherm can crack a 50 mm block.
• High fracture toughness: the tight saturated network is brittle, so blend it or move to an aromatic system.
Incoming inspection covers EEW, total chlorine and colour. EEW by titration according to ASTM D1652 catches a blended or aged drum; chlorine above 50 ppm matters for electrical work; colour drift points to oxidation.
The grade ships in drums and IBC tanks and keeps 24 months between 5 and 30 °C, away from sunlight, oxidants and acids. Handling data sits in the MSDS, lot values in the COA. Values here describe the grade, not one drum.
Alicyclic. Both epoxy groups sit inside cyclohexane rings joined by an ester bridge, so no glycidyl ether tail is present and total chlorine stays at or below 50 ppm.
Anhydrides and cationic initiators. MHHPA runs 106–135 phr across the EEW window, and a photoacid serves UV cure. Aliphatic amines react too slowly at room temperature.
Water, amine contamination or oxygen inhibition. Dry the resin below 0.05% water, clean the mixer between product families, and cure under nitrogen if the surface must come out hard.
Up to about 30% by weight. Expect 370 mPa·s at 10% and 820 mPa·s at 30%, with blend EEW rising from 130 to 143 g/eq.
Several days at 25 °C and weeks at 5 °C. The mix stays latent until roughly 120 °C, which suits one-shot casting.
Sealed between 5 and 30 °C, out of sunlight, 24 months from manufacture. A drum opened repeatedly picks up moisture, so purge the headspace with dry air before closing it.
YLCE-2021 is a low-viscosity alicyclic diepoxide: 125–135 g/eq, 200–300 mPa·s at 25 °C, 50 ppm total chlorine, and a colourless body that resists yellowing under UV.
Stoichiometry is the easy part. MHHPA at 110 phr covers the mid-point EEW, DETA at 15.8 phr works only in an oven, and 10% bisphenol A is about all the flow window takes.
Cure chemistry is the hard part. Cationic systems fail on trace moisture and amine, and the failure looks like a tacky skin. Cast a coupon before the production mould is cut.
1. Yolatech product page, YLCE-2021: https://www.yolatech.com/34-epoxycyclohexylmethyl-ylce-2021-cas-2386-87-0
2. Yolatech product page, YLCE-186: https://www.yolatech.com/45-epoxytetrahydrophthalic-acid-diglycidylester-ylse-186-cas-25293-64-5
3. Yolatech product page, bisphenol A grades: https://www.yolatech.com/bisphenol-a-epoxy-resin
4. Yolatech product page, MHHPA: https://www.yolatech.com/34-methyl-hexahydrophthalic-anhydride-cas-no-25550-51-0-mhhpa
5. Technical Data Sheet, Material Safety Data Sheet and Certificate of Analysis (COA) for YLCE-2021, CAS 2386-87-0, Yolatech (available on request).
6. ASTM D1652, epoxy content of epoxy resins; ISO 3001, determination of epoxy equivalent.
7. ASTM D445, kinematic viscosity; ASTM D1544, Gardner color; ASTM E203, water by Karl Fischer; ASTM D93, flash point by Pensky-Martens.